Anodising and Finishes for Aluminium Machined Parts: What to Specify
Finish specifications are frequently copied from an older drawing. The result is either a part that fails corrosion testing or a part that no longer fits its mating thread. These are the parameters that decide both.
Type II versus Type III
Type II sulfuric anodising builds 5-25 µm and is the decorative and general-corrosion finish. Type III hard anodising builds 25-50 µm with much higher wear resistance, and is darker and more brittle at the edges. Hard anodising on sharp corners will chip; specify a radius before you specify Type III.
Thickness and dimensional growth
Anodic film grows roughly half outward and half inward. A 20 µm film adds about 10 µm per surface - 0.02 mm on a diameter. On an H7 bore or a precision shaft this matters. Either pre-machine to allow for growth or mask the feature.
| Process | Typical film | Growth per surface |
|---|---|---|
| Type II clear | 10-20 µm | ~5-10 µm |
| Type III hard | 25-50 µm | ~12-25 µm |
| Chemical conversion (Alodine) | 0.3-1 µm | negligible |
Masking threads, holes and contacts
Threads must be masked or re-tapped after anodising; film in a thread destroys the fit. Specify masking for grounding points, connector bores and any surface that will be bonded. Masking is manual work priced per feature - fewer masked features means a lower price.
Colour matching
Black and clear are stable. Colours are dye lots: two batches of the same nominal colour will not match exactly, and anodising a small batch to a Pantone reference is not realistic. If colour consistency matters, define a numeric tolerance (for example a Delta E limit) against a master plaque rather than a colour name.
Mechanical preparation
As-machined surfaces show tool marks through a thin film. Bead blasting gives an even matte that hides them; brushing gives a directional finish that must be specified per face. Blasting also removes edge sharpness, which can be desirable or not.
Other finishes worth considering
- Powder coating: 60-100 µm, excellent outdoors, needs masking or an earth path.
- Passivation: for stainless, not aluminium - removes free iron after machining.
- Zinc or zinc-nickel plating: for steel fasteners and brackets that must survive salt spray.
- Chemical conversion coating: cheap, conductive, good paint base, minimal dimensional change.
Test requirements
If the application needs corrosion evidence, state the test: neutral salt spray hours, film thickness method, and adhesion (tape or bend test). Without a test clause, "anodised" means appearance only and cannot be rejected on performance.